Material: | Titanium |
Method Used: | Annealing |
Depth: | Surface |
Laser Type: | Pulsed Fiber |
Focal Length Lens: | 160mm |
Power: | 95% |
Frequency: | 30 kHz |
Speed: | 1″ per sec |
Passes: | 12 |
Cycle Time: | 26.52 seconds |
The samples were processed using the 20 watt Pulsed Fiber Laser equipped with a 160mm lens. In order to get the marks darker than what was currently being produced the beam was defocused approximately 6mm above the part. A low frequency was used to obtain the highest amount of beam intensity and a slow mark speed was used. The parameters that produced the best results were marking at 6mm above focus, 95% Power, 30 kHz and 1 “ per second mark speed. The mark darkens more and more with each consecutive pass, using 10-12 passes produced the best results during testing.